Aluminum
- Aluminum
-
Stainless Steel
- Stainless Steel
-
Steel
- Steel
-
Red Metals
- Red Metals
-
Other Metals
- Other Metals
-
Plastics
- Plastics
-
Composites
- Composites
-
Rubber
- Rubber
-
Framing Systems
- Framing Systems
-
Precision Products
- Precision Products
-
3D Printing
- 3D Printing
-
Fittings
- Fittings
Open for Orders 24/7!
- Home
- product guide
- Alloy
A2 Product Guide
Applications | Specifications | Mechanical and Chemical Data | Tolerances
Overview
An air-hardening tool steel with good strength and with excellent stability in heat treatment. A-2 exhibits wear resistance that falls between O-1 and D-2 steel. Typically used in punches, dies, cutting tools in woodworking, tooling for plastic, dowel pins, hammers, and industrial knives.
Common Trade Names
UNS T30102, AISI Type A2, AISI Medium-Alloy, Air-Hardening Tool Steels A2, Air-True
Other Resources
Weight Calculator | Mill Test Reports
Products
A2 Drill Rod | A2 Rectangle Bar | A2 Square Bar
Applications
- Dowel Pins
- Blades
- Punches
- Dies
- Tooling
- Hammers
Specifications
ASTM | SAE |
---|---|
A681 | J437 |
A-2 Tool Steel Heat Treatment | ||||
Hardness | Heat Treat Temp. | Quench Medium | Applications | Advantages |
---|---|---|---|---|
As Shipped: Rockwell 94-99B
After Heat Treating: Rockwell 59-62C | 1700°-1900°F | Air | A2 can be used in the same applications as both O1 and W1. | The heat-treated air-hardening steels have deeper hardenability and there is less movement or distortion during heat treatment. |
Physical Properties A2 | |||||
Annealed | Hardened | ||||
---|---|---|---|---|---|
Density | 0.284 lb/in3 | 0.284 lb/in3 | |||
Ultimate Tensile Strength | 100 ksi | 300 ksi | |||
Yield Tensile Strength | 50 ksi | N/A | |||
Shear Modulus | 11,300 ksi | 11,300 ksi | |||
Shear Strength | 65 ksi | N/A | |||
Fatigue Strength | 35 ksi | N/A | |||
Hardness Rockwell | Brinell | B94-99 | 200-235 | C59-62 | 634-688 | |||
Elongation at Break Percentage | 21% | N/A | |||
Modulus of Elasticity | 29,400 ksi | 29,400 ksi | |||
Poisson's Ratio | 0.30 | 0.30 | |||
Machinability Percentage | 65% | 65% | |||
Melting Point | 2,570-2,650 °F | 2,570-2,650 °F | |||
Specific Heat | 1.1 x 10^-1 BTU/lb-°F | 1.1 x 10^-1 BTU/lb-°F | |||
Thermal Conductivity | 264 BTU-in/hr-ft^2-°F | 264 BTU-in/hr-ft^2-°F | |||
Electrical Conductivity | 8.2% IACS | 8.2% IACS |
Chemistry Information
|
|
Element |
Percentage |
C | 0.95 - 1.05 |
Cr | 5.13 |
Fe | 91 |
Mn | 1 max |
Mo | 1.15 |
P | 0.03 max |
Si | 0.5 max |
S | 0.03 max |
V | 0.33 |