☆ Double Points for Dads! ☆
Rewards Members Earn 2X Points on Qualifying Purchases Until 6/15 at Midnight!
Rewards Members Earn 2X Points on Qualifying Purchases Until 6/15 at Midnight!
Applications | Specifications | Related Videos | Mechanical and Chemical Data | Tolerances
6262 aluminum was designed for operations where significant machining is required. It contains lead and bismuth to help with chip creation and breakage, as well as to partially lubricate the cutting tool. 6262 is generally regarded as having good strength and corrosion resistance. Finished parts can be produced with a high level of polishing. It is typically used in camera parts, couplings, marine fittings, decorative hardware, hinge pins, knobs, nuts, oil line fittings, appliance fittings, valves and valve parts.
UNS A96262, ISO AlMg1SiPb, AA6262-T6511, Al6262-T6511
Safety Data Sheet | Weight Calculator | Mill Test Reports
Purchase Hex Bar 6262 | Round Bar 6262
ASTM |
---|
B221 |
Physical Properties 6262 | |||||
-T6511 | |||||
---|---|---|---|---|---|
Density | 0.098 lb/in3 | ||||
Ultimate Tensile Strength | 43 ksi | ||||
Yield Tensile Strength | 39 ksi | ||||
Fatigue Strength | 15 ksi | ||||
Shear Strength | 26 ksi | ||||
Shear Modulus | 3,700 ksi | ||||
Hardness Rockwell | Brinell | B36 | 71 | ||||
Elongation at Break Percentage | 10% | ||||
Modulus of Elasticity | 9,900 ksi | ||||
Poisson's Ratio | 0.33 | ||||
Machinability Percentage | 70% | ||||
Melting Point | 1,080-1,205 °F | ||||
Specific Heat | 2.1 x 10^-1 BTU/lb-°F | ||||
Thermal Conductivity | 1,188 BTU-in/hr-ft^2-°F | ||||
Electrical Conductivity | 44% IACS |
Chemistry Information
|
|
Element |
Percentage |
Al | 94.6 - 97.8 |
Bi | 0.4 - 0.7 |
Cr | 0.04 - 0.14 |
Cu | 0.15 - 0.4 |
Fe | 0.7 max |
Pb | 0.4 - 0.7 |
Mg | 0.8 - 1.2 |
Mn | 0.15 max |
Si | 0.4 - 0.8 |
Ti | 0.15 max |
Zn | 0.25 max |