Aluminum 1100 Product Guide
Applications | Specifications | Mechanical and Chemical Data | Tolerances
Overview
1100-H14 aluminum is usually what is meant by "commercial grade aluminum". It is known for its superior corrosion resistance, formability, conductivity, and high weldability. It is not used in applications that require high strength or hardness. 1100 is nonmagmetic, weldable, and not heat treatable.
1100 is typically used for chemical equipment, food handling equipment, decorative trim, lighting equipment, and heat exchangers. If excellent malleability and corrosion resistance are your primary goals, 1100-H14 is an excellent choice.
Common Trade Names
UNS A91100, ISO Al99.0Cu, AA1100-H14, Al1100-H14
Other Resources
Safety Data Sheet | Weight Calculator | Mill Test Reports
Products
Applications
- Chemical Equipment
- Food Handling Equipment
- Decorative Trim
- Lighting Equipment
- Heat Exchangers
Aluminum 1100 Specifications
ASTM | AMS | ASME |
---|---|---|
B209 | QQ-A-225/1 | SFA5.10 |
B210 | QQ-A-250/1 | SFA5.3 |
B211 | 4003 | |
B221 | 7220 | |
B247 | QQ-A-430 | |
B313 | QQ-WW-T-700/1 |
Physical Properties 1100 | |||
-O | -H14 | -H112 | |
---|---|---|---|
Density | 0.1 lb/in3 | 0.1 lb/in3 | 0.1 lb/in3 |
Ultimate Tensile Strength | 13 ksi | 16-21 ksi | min. 12 ksi |
Yield Tensile Strength | 5 ksi | 17 ksi | 5.2 ksi |
Fatigue Strength | 5 ksi | 7 ksi | 4.6 ksi |
Shear Strength | 9 ksi | 11 ksi | 7.8 ksi |
Shear Modulus | 3,770 ksi | 3,770 ksi | 3,770 ksi |
Hardness Rockwell | Brinell | N/A | 23 | N/A | 32 | N/A | 23 |
Elongation at Break Percentage | 32% | 1-10% | min. 14% |
Modulus of Elasticity | 10,000 ksi | 10,000 ksi | 10,000 ksi |
Poisson's Ratio | 0.33 | 0.33 | 0.33 |
Machinability Percentage | 10% | 30% | N/A |
Melting Point | 1,190-1,215 °F | 1,190-1,215 °F | 1,190-1,210 °F |
Specific Heat | 2.2 x 10^-1 BTU/lb-°F | 2.2 x 10^-1 BTU/lb-°F | 2.2 x 10^-1 BTU/lb-°F |
Thermal Conductivity | 1,560 BTU-in/hr-ft^2-°F | 1,560 BTU-in/hr-ft^2-°F | 1,560 BTU-in/hr-ft^2-°F |
Electrical Conductivity | 59% IACS | 59% IACS | 59% IACS |
Chemistry Information
|
|
Element |
Percentage |
Al | 99 min |
Cu | 0.5 - 2 |
Mn | 0.05 max |
Si+Fe | 0.95 max |
Zn | 0.1 max |