Copper 110 Product Guide
Applications | Specifications | Mechanical and Chemical Data | Tolerances
Overview
Most commonly known for its sublime electrical and thermal conductivity and formability. Additionally, 110 copper has good corrosion resistance and has excellent hot and cold workability. Brazing is rated as good, soldering as excellent. 110 can be welded with precautions, but generally the sorts of inert gases required are not recommended for use with coppers. Having a variety of purposes, Copper 110 is typically used anywhere from plumbing hardware, wiring and electrical components to telecommunication materials.
Common Trade Names
UNS C11000, CDA 110 ETP, C110, ISO Cu-ETP, Electrolytic Tough Pitch
Other Resources
Safety Data Sheet | Weight Calculator | Mill Test Reports
Products
Purchase Full Round Edge Rectangle Bar 110 | Rectangle Bar 110 | Round Bar 110 | Square Bar 110 | Foil 110 | Sheet/Plate 110 | Sample Pack 110 | Tape 110 | Threaded Rod 110 | Shim Stock 110
Applications
- Plumbing Hardware
- Wiring
- Electronics
- Decorative Hardware
- Telecommunications
Copper 110 Specifications
ASTM |
---|
B187 |
Physical Properties 110 | |||||
-O/Annealed | -H00 | -H01 | -H02 | -H04 | |
---|---|---|---|---|---|
Density | 0.321 lb/in3 | 0.321 lb/in3 | 0.321 lb/in3 | 0.321 lb/in3 | 0.321 lb/in3 |
Ultimate Tensile Strength | 32 ksi | 36 ksi | 38 ksi | 42 ksi | 50 ksi |
Yield Tensile Strength | 10 ksi | 28 ksi | 30 ksi | 36 ksi | 45 ksi |
Shear Strength | 22 ksi | 25 ksi | 25 ksi | 26 ksi | 28 ksi |
Shear Modulus | 6,300 ksi | 6,300 ksi | 6,300 ksi | 6,300 ksi | 6,300 ksi |
Hardness Rockwell | Brinell | B10 | 57 | B10 | 57 | B25 | 64 | B40 | 74 | B50 | 83 |
Elongation at Break Percentage | 55% | 33% | 22% | 14% | 20% |
Modulus of Elasticity | 17,000 ksi | 16,700-18,900 ksi | 16,700-18,900 ksi | 16,700-18,900 ksi | 16,700-18,900 ksi |
Poisson's Ratio | 0.34 | 0.34 | 0.34 | 0.34 | 0.34 |
Machinability Percentage | 20% | 20% | 20% | 20% | 20% |
Melting Point | 1,949-1,981 °F | 1,949-1,981 °F | 1,949-1,981 °F | 1,949-1,981 °F | 1,949-1,981 °F |
Specific Heat | 9.2 x 10^-2 BTU/lb-°F | 9.2 x 10^-2 BTU/lb-°F | 9.2 x 10^-2 BTU/lb-°F | 9.2 x 10^-2 BTU/lb-°F | 9.2 x 10^-2 BTU/lb-°F |
Thermal Conductivity | 2690 BTU-in/hr-ft^2-°F | 2690 BTU-in/hr-ft^2-°F | 2690 BTU-in/hr-ft^2-°F | 2690 BTU-in/hr-ft^2-°F | 2690 BTU-in/hr-ft^2-°F |
Electrical Conductivity | 100% IACS | 100% IACS | 100% IACS | 100% IACS | 100% IACS |
Chemistry Information
|
|
Element |
Percentage |
Cu | 99.9 |
O | 0.04 |